Home / Insights / Insights

Corrosion pits, fatigue and a fractured landing gear leg: lessons for any cyclically loaded steel part

On 30 June 2025 the left landing gear leg of a light aerobatic aircraft fractured as it touched down at Tatenhill Aerodrome in Staffordshire. The aircraft ran off onto the grass and both occupants were unhurt. The UK Air Accidents Investigation Branch (AAIB) published its report on 14 May 2026 (read the report).

The aircraft is a small one, but the failure sequence is one we see in industrial plant: a protective coating is damaged, corrosion starts, a fatigue crack grows from the corrosion, and the part finally breaks under a load it had carried many times before.

What happened

The gear leg is a high-strength steel spring leg. According to the AAIB:

The AAIB concluded that the leg failed in overload on touchdown, after fatigue cracks had grown from where surface corrosion developed.

The maintenance gap

In 2018 the manufacturer issued a service letter (SL-449) on corrosion inspection and preventative maintenance. It recommended visual inspection of the gear legs for corrosion at intervals set by the local corrosion environment. The service letter was not mandatory under the aircraft's approved maintenance programme. The AAIB could not say whether following it would have found the damage in time. It did note that operators may wish to include it in their programmes.

Lessons for plant and asset owners

1. Coating damage on stressed steel is a structural finding. High-strength steels are sensitive to surface defects. Once the coating is gone, corrosion pits create the stress concentrations that fatigue cracks need.

2. Corrosion and fatigue interact. A pit a millimetre or two deep would rarely matter for static strength. Under cyclic loading it can be where a crack starts. Shafts, bolts, springs, lifting equipment, pump and fan components, and structural brackets are all exposed to the same mechanism.

3. The fracture surface tells the story. Fractography separates a single overload from a crack that grew over months or years. That is the difference between "the load was too high" and "the inspection regime missed a growing defect", and each needs a very different corrective action.

4. Guidance only works once it is in the programme. Manufacturer letters, bulletins and industry alerts need a route into your inspection plan, with an owner and an interval.

What to check on your own components

How MTIS can help

MTIS carries out failure investigations on metallic components, including fractography, metallography and corrosion assessment. We identify the mechanism and the root cause, and recommend practical changes to inspection and maintenance. If you have a failed part, or a population of similar parts you are worried about, contact MTIS to discuss it.

Source: UK Air Accidents Investigation Branch, report on Bellanca (American Champion) Decathlon 8KCAB, G-TALX, published 14 May 2026. This article summarises the public report in our own words; see the original for full details.

What the MTIS Failure Investigation Assistant concluded

We put the report's own observations into our Failure Investigation Assistant: a steel landing gear leg, fractured at the bend, with fatigue cracking on the fracture surface and corrosion at the initiation site. It ranked corrosion fatigue first, matching the AAIB's finding, and did so from the report alone before the laboratory detail was added. It flagged its own confidence in that answer as low, which is the honest reading of evidence this thin - a diagnosis worth confirming by fractography, not a conclusion to act on.

Try the Failure Investigation Assistant